Reference Last checked November 19, 2026
Arc Bead vs. Fire Melting: What the Research Shows
The features investigators use to tell an arc bead from fire melting and alloying on copper wire, drawn from the published research, with the points where it disagrees.
An arc bead is a melted spot on a conductor left by electrical arcing; fire melting is copper or aluminum melted by the heat of the fire; alloying is copper mixed with another metal, such as aluminum or zinc, at high temperature. Investigators tell them apart by the shape and extent of the melting, the boundary with the unmelted wire, the inside of the melted metal and where the damage sits in the building. Published research disagrees on how reliably this can be done by eye.
This page sets out the features as the sources describe them, with drawings instead of photographs. Last checked: November 19, 2026.
The features, side by side
- A clean bead on the severed end, with a sharp line where it meets the wire.
- A matching notch on the neighboring conductor at the same spot.
- Drawing lines from manufacture run up to the site and stop there.
- The wire keeps its full diameter right up to the damage: the site is localized.
- The wire thins gradually over a length (necking), with no sharp line.
- Irregular globules with a non-uniform surface.
- Drips where the melted metal ran down.
- Drawing lines melted away well back from the site.
- Copper mixed with aluminum: a silver-colored region where the two touched.
- The other metal (here an aluminum part) in contact with the copper.
| Feature | Arc melt site | Fire melt site | Alloying site |
|---|---|---|---|
| Form | Beads or notches; may include welding or severing of the conductors | Gross melting, globules or balls | Mixing of dissimilar metals at the damage site |
| Surface | In part a smooth surface | A non-uniform surface and shape | With aluminum, silver in color; with zinc, bronze |
| Boundary | Distinct lines of demarcation | No clear lines of demarcation | Visually distinguishable from arc melt sites of copper only |
| Extent | Localized | Irregular melting in and around the site; multiple or widespread areas | A subset of fire melting |
| Drawing lines from manufacture | Obliterated within the site; may remain outside it | Generally melted at and away from the site | Not described in the source |
| Inside the melted metal | Internal uniform porosity | No porosity, or non-uniform porosity | Not described in the source |
Source of the table: the damage types “generally recognized” in Svare, Hanke and Nic Daeid, Journal of the National Academy of Forensic Engineers, June 2023. The paper adds that arc melt sites are made by electricity, not by fire.
Can they be told apart by eye?
The same NAFE paper reports a survey of 317 participants who could reliably identify mechanical damage but had a low probability overall (45.61 %) of visually distinguishing arc melting from fire melting.
A study funded by the National Institute of Justice (Roby and McAllister, 2012) tested more than 190 wires, energized and not energized, under flame, radiant and flashover exposures. Round copper globules with clear lines of demarcation, traditionally called beads, formed on both energized and non-energized wires, and the authors found no visual or microscopic trait that set the two apart. They concluded that using visual characteristics alone to establish whether a wire was energized can lead to erroneous conclusions.
The NIJ report quotes the 2011 edition of NFPA® 921, which defined a bead as a round globule caused by arcing and characterized by a sharp line of demarcation, and says the guide needed revision in light of its findings. NFPA® 921 is sold by the NFPA®, so this page does not quote later editions.
A measurement instead of a judgment
- A: arc melting. In the 2023 tests the displaced copper stayed within four conductor diameters (CD) of the site.
- B: fire melting. The displaced copper reached beyond four conductor diameters.
Svare, Hanke and Nic Daeid ran 63 full-scale compartment fires at the federal law enforcement training center in Brunswick, Georgia, on 14 AWG copper cable, plus scaled tests on UK cable of 1.0 and 2.5 mm². In their tests, arc melt sites were found only on energized circuits and only within the area of origin. They measured how far melted copper was displaced along the conductor: arc melting stayed within four times the conductor diameter, and fire melting went beyond it, at 95 % across their data set. They note that other conductor sizes, materials and fault currents may need more testing.
Inside the bead: what a laboratory adds
- Arc bead in section: an abrupt change of grain size where bead meets wire (an internal line of demarcation). NIJ found it in 40 % of energized beads and in one non-energized bead.
- Internal uniform porosity, described for arc melt sites and best seen in a metallographic section.
- Fire melting in section: a gradual change from melted to wire grain structure.
- No porosity, or non-uniform porosity.
- Sectioning. The NAFE paper notes that light microscopy or SEM of the surface may not reveal internal porosity that is easily seen in a properly prepared metallographic section, and cites earlier work describing a “Swiss cheese” porosity in arc melted copper.
- Grain structure. NIJ found an internal line of demarcation, an abrupt change of grain size between bead and wire, in 40 % of the energized beads and in one non-energized bead, so neither its presence nor its absence proves the energized state.
- Chemistry. In an EC&M article, a consultant describes Auger electron spectroscopy of a bead, reasoning that a bead formed in a fire traps combustion products and one formed before the fire does not. The NIJ study found no trends in grain structure or chemical composition between energized and non-energized samples with SEM and EDS.
- Methods used. The NAFE study examined its samples by visual examination, measurement, light microscopy, SEM/EDS, X-ray and metallographic examination; our article on X-ray inspection in forensics explains the X-ray step.
Alloying, and when it is eutectic
The NAFE paper calls the mixing of dissimilar metals at high temperature alloying, a subset of fire melting, and notes that “eutectic” is a specific term: some mixtures, such as copper and aluminum, have a eutectic, while others, such as copper and zinc, do not. Our eutectic melting calculator shows the temperatures at which these mixtures start to melt, and the article on eutectic melting of copper and aluminum in fires covers the topic in more depth.
Where it fits in an investigation
A single bead is one piece of evidence. Arc mapping records every arc site on the circuits in the fire area; our article on common myths about arc mapping covers its limits, and arcing vs. melting damage gives the short version of this page with an interactive drawing. The fire investigation guide lists the rest of our fire articles in reading order, and our electrical fire investigation page describes the service.
Where the sources disagree
| Question | One view | Another view |
|---|---|---|
| Does a bead show the wire was energized? | NIJ (2012): beads formed on energized and non-energized wires; visual features alone can mislead. | NAFE (2023): in its tests arc melt sites appeared only on energized circuits, and a measurement separated arc from fire melting. |
| Can the inside of a bead be read? | NIJ: no definitive trait; an internal line of demarcation in 40 % of energized beads and in one non-energized bead. | NAFE: SEM, EDS and microstructure analysis further supported telling arc from fire melting in its data. |
| Does bead chemistry show which came first? | EC&M (Anderson): Auger electron spectroscopy shows whether combustion products were trapped. | NIJ: no trends in chemical composition with SEM and EDS. |
The studies differ in wire sizes, fire exposures and how energized wires were loaded, and the NAFE authors write that the NIJ report and a 2012 thesis by Hussain present the same data under different authorship.
Method and sources
- Free sources only, read on November 19, 2026. NFPA® 921 is not quoted beyond the 2011 definition cited in the NIJ report.
- The drawings are ours, made from the sources’ written descriptions. They are schematic, not to scale, and show no case evidence.
- Where sources disagree, both are given with the conditions of each study.
Sources
- R. J. Roby and J. McAllister, Forensic Investigation Techniques for Inspecting Electrical Conductors Involved in Fire, final report, NIJ award 2010-DN-BX-K246, document 239052, July 2012 (opens in a new tab). Federally funded grant report made available by NCJRS; not published by the Department of Justice.
- M. J. Svare, N. W. Hanke and N. Nic Daeid, Forensic Examination of Post-Fire Damaged Electrical Conductors by Quantitative Measurement, Journal of the NAFE 40(1), June 2023. Free to read; copyright NAFE. Quoted briefly for its findings.
- R. N. Anderson, What Came First: The Arc Bead or the Fire?, EC&M, July 1, 2001 (opens in a new tab). Trade article by a consultant; free to read.
Changes
- November 19, 2026: first published.
Frequently asked questions
What is an arc bead?
A melted spot on a conductor left by electrical arcing. The features usually described are a round bead or notch, a smooth surface, a sharp line between melted and unmelted metal, and damage confined to one spot.
Can fire alone make a bead on a copper wire?
Yes. A study funded by the National Institute of Justice produced round copper globules with clear lines of demarcation on wires that were not energized.
How do investigators tell arcing from fire melting?
They look at the shape and extent of the melting, the boundary with the sound wire, drawing lines, porosity in a metallographic section and where the site is relative to the area of origin. One 2023 study proposes measuring how far melted copper is displaced along the wire.
Is alloying the same as eutectic melting?
Not always. Alloying is any mixing of dissimilar metals at high temperature. Eutectic melting applies only to alloy systems that have a eutectic, such as copper and aluminum; copper and zinc do not.
Questions about a fire, a code or corrosion data?
Our licensed Professional Engineers investigate fires and electrical failures and review corrosion data.