Free tool screening estimate
ISO 9223 Corrosivity Category From First-Year Corrosion
Places a first-year mass or thickness loss of steel or zinc in the EN ISO 9223 corrosivity categories C1 to CX.
Tool referenceDE-TOOL-10858
- Method
- EN ISO 9223 first-year limits, as reproduced in Materials 14 (2021) 5219
- Metals
- Low-carbon steel, zinc
- Output
- Category C1 to CX
ISO 9223 rates the corrosivity of an atmosphere from C1 (very low) to CX (extreme). With a first-year result, the category is a lookup: for low-carbon steel, a first-year mass loss above 200 and up to 400 g/m², or a thickness loss above 25 and up to 50 µm, is C3 (medium). This tool does that lookup for steel and zinc, with the limits of EN ISO 9223 as reproduced in an open-access paper.
ISO 9223 corrosivity category from a first-year result
Enter the first-year corrosion of a low-carbon steel or zinc specimen, as mass loss, thickness loss, or a coupon's mass loss and area. The tool places it in the EN ISO 9223 categories C1 to CX. The answer updates as you type.
The tool needs JavaScript®. The category table it uses is on this page.
Quick start Fills in the form. Change anything after.
Result
C3: Medium corrosivity
320 g/m² on low-carbon steel falls in C3 (Medium), the band above 200 and up to 400 g/m².
Mass loss and thickness loss are separate columns in the source; the tool uses the column you entered and does not convert between them.
- Category
- C3
- Corrosivity
- Medium
- Value used
- 320 g/m²
A category describes the atmosphere at one site for one year. It is not a coating design or a service life. See corrosion engineering, or ask an engineer.
EN ISO 9223 first-year categories: Bands for low-carbon steel
| Category | Corrosivity | Mass loss, g/m² | Thickness loss, µm |
|---|---|---|---|
| C1 | Very low | ≤ 10 | ≤ 1.3 |
| C2 | Low | > 10 to ≤ 200 | > 1.3 to ≤ 25 |
| C3 | Medium | > 200 to ≤ 400 | > 25 to ≤ 50 |
| C4 | High | > 400 to ≤ 650 | > 50 to ≤ 80 |
| C5 | Very high | > 650 to ≤ 1,500 | > 80 to ≤ 200 |
| CX | Extreme | > 1,500 to ≤ 5,500 | > 200 to ≤ 700 |
Full results and steps
| Metal | low-carbon steel |
|---|---|
| Column used | Mass loss, g/m² |
| Value | 320 g/m² |
| Category | C3 (Medium) |
- 320 g/m² is above 200 and not above 400: C3.
Choosing a coating or a corrosion allowance?
Dreiym's licensed Professional Engineers assess atmospheric corrosion at plants, pipelines and structures.
Assumptions and limits
Assumptions: a specimen of the standard metal exposed for its first year at the site, with the corrosion products removed before weighing.
What this does not do: it does not estimate a category from time of wetness, sulfur dioxide or chloride deposition, and it does not cover copper or aluminum. The free sources we found did not give those tables with their units.
Screening tool: For education and planning. Not a site classification under the standard, and not a substitute for a licensed engineer's review.
How the calculation works
- Each category is a band of first-year loss: above the lower limit, up to and including the upper limit.
- Mass loss and thickness loss each have their own limits for steel and for zinc.
- A coupon result is divided by its area (10,000 cm² in 1 m²) to give g/m².
Sources
Sources: M. Šmak and J. Kubíček, The Influence of Hot-Dip Galvanizing on the Mechanical Properties of High-Strength Steels, Materials 14 (2021) 5219, Table 1, which reproduces the first-year values of EN ISO 9223 (CC BY 4.0); ISO 9223:2012, Corrosion of metals and alloys, Corrosivity of atmospheres, Classification, determination and estimation (sold by ISO; not read).
Cite or share this tool
Dreiym Engineering. ISO 9223 corrosivity category. Limits: EN ISO 9223 first-year values as reproduced in Smak and Kubicek, Materials 14 (2021) 5219, Table 1. https://www.dreiym.com/iso-9223-corrosivity-category/
Instructors and shops are welcome to link to this tool or put its address on a handout. It is free, needs no sign-up and works on a phone.
Link copied.Citation copied.The copy did not work. The text is selected, so copy it with your device.AccessedHow to use the tool
Choose steel or zinc, then enter the first-year result as a mass loss per area, a thickness loss, or a coupon’s mass loss with its exposed area and exposure time. The result names the category and shows where the value falls among the six bands.
How to find the corrosivity category from a first-year result
- Expose a specimen for one year. A low-carbon steel or zinc specimen at the site, for the first year.
- Remove the corrosion products and weigh it. The mass lost, divided by the exposed area in m², is the mass loss in g/m².
- Find the band. Each category runs from above its lower limit up to and including its upper limit.
- Read the category. C1 very low, C2 low, C3 medium, C4 high, C5 very high, CX extreme.
The first-year limits
| Category | Corrosivity | Steel, g/m² | Steel, µm | Zinc, g/m² | Zinc, µm |
|---|---|---|---|---|---|
| C1 | Very low | ≤ 10 | ≤ 1.3 | ≤ 0.7 | ≤ 0.1 |
| C2 | Low | > 10 to ≤ 200 | > 1.3 to ≤ 25 | > 0.7 to ≤ 5 | > 0.1 to ≤ 0.7 |
| C3 | Medium | > 200 to ≤ 400 | > 25 to ≤ 50 | > 5 to ≤ 15 | > 0.7 to ≤ 2.1 |
| C4 | High | > 400 to ≤ 650 | > 50 to ≤ 80 | > 15 to ≤ 30 | > 2.1 to ≤ 4.2 |
| C5 | Very high | > 650 to ≤ 1,500 | > 80 to ≤ 200 | > 30 to ≤ 60 | > 4.2 to ≤ 8.4 |
| CX | Extreme | > 1,500 to ≤ 5,500 | > 200 to ≤ 700 | > 60 to ≤ 80 | > 8.4 to ≤ 25 |
First year of exposure. Source: Šmak and Kubíček, Materials 14 (2021) 5219, Table 1, “The corrosion rate of steel and zinc with respect to corrosivity categories (EN ISO 9223)”.
Worked example
A steel coupon loses 0.64 g from 20 cm² in its first year. That is 0.64 ÷ 20 × 10,000 = 320 g/m². 320 is above 200 and not above 400, so the site is C3, medium corrosivity, for that year.
What this tool does not do, and why
ISO 9223 also estimates the category without a specimen, from the environment: dose-response functions that use temperature, relative humidity, and sulfur dioxide and chloride deposition. The standard is sold by ISO. The free sources we found give such functions, for example a table of published functions for carbon steel in Chico and others (Materials 2017), but they do not state the units of each term or present them as the standard’s own functions, and none gave the limits for copper or aluminum. Rather than guess, the tool leaves these out.
A category describes one site over one year. For how humidity, salt and pollutants drive the loss, see our article on atmospheric corrosion; to convert a first-year loss between units, use the corrosion rate converter.
Verified against
The limits in the tool are the source table, checked value by value. At every limit the tool gives the lower category, and just above it the next one: 24 limits for steel and zinc, in both columns, 48 checks in all, plus the coupon arithmetic of the worked example. No free source we found reports a published first-year result together with its category, so there is no external worked case to compare with.
Checks against the source table
| What is checked | Source | Tool |
|---|---|---|
| Steel 200 g/m², the upper limit of C2 | C2 | C2 |
| Steel just above 200 g/m² | C3 | C3 |
| Steel 1,500 g/m², the upper limit of C5 | C5 | C5 |
| Zinc 2.1 µm, the upper limit of C3 | C3 | C3 |
| Steel 6,000 g/m², above CX | Above the table | Above the table |
| Coupon 0.64 g on 20 cm² | 320 g/m² (by hand) | 320 g/m², C3 |
Method and sources
- M. Šmak and J. Kubíček, The Influence of Hot-Dip Galvanizing on the Mechanical Properties of High-Strength Steels, Materials 14 (2021) 5219, Table 1. Open access, CC BY 4.0. The table reproduces the first-year values of EN ISO 9223.
- B. Chico and others, Annual Atmospheric Corrosion of Carbon Steel Worldwide, Materials 10 (2017) 601, Table 8. Open access, CC BY 4.0. Cited for the published dose-response functions it lists; not used in the tool.
- ISO 9223:2012, Corrosion of metals and alloys, Corrosivity of atmospheres, Classification, determination and estimation. Sold by ISO; not read.
Licence notes: both papers are CC BY 4.0, which allows the values to be restated with attribution, as here. The tool and page copy no text of the standard.
Frequently asked questions
What are the ISO 9223 corrosivity categories?
Six categories of atmospheric corrosivity: C1 very low, C2 low, C3 medium, C4 high, C5 very high and CX extreme, each defined by the first-year corrosion of standard metals.
What first-year steel loss is C5?
Above 650 and up to 1,500 g/m² of mass loss, or above 80 and up to 200 µm of thickness loss, for low-carbon steel in its first year.
Can I use a result from a six-month exposure?
The table is for the first year of exposure. The tool scales a shorter or longer exposure to a year for information, and says the category is then not a first-year result.
Why is there no estimate from humidity and salt?
ISO 9223 gives dose-response functions for that, but the standard is sold by ISO and the free sources we found do not give those functions with their units. The tool uses only the first-year table.
More engineering tools
All calculatorsNeed more than a screening estimate?
We typically respond within one business day.